{"id":4239,"date":"2026-06-03T01:42:38","date_gmt":"2026-06-03T01:42:38","guid":{"rendered":"https:\/\/wolorin.com\/?page_id=4239"},"modified":"2026-06-10T03:26:33","modified_gmt":"2026-06-10T03:26:33","slug":"heat-pressure-rubber-rollers","status":"publish","type":"post","link":"https:\/\/wolorin.com\/es\/blog\/heat-pressure-rubber-rollers\/","title":{"rendered":"How to Choose Rubber Rollers for Heat and Pressure Contact"},"content":{"rendered":"<div data-elementor-type=\"wp-page\" data-elementor-id=\"4239\" class=\"elementor elementor-4239\">\n\t\t\t\t<div class=\"elementor-element elementor-element-6922788c e-flex e-con-boxed e-con e-parent\" data-id=\"6922788c\" data-element_type=\"container\" data-e-type=\"container\">\n\t\t\t\t\t<div class=\"e-con-inner\">\n\t\t\t\t<div class=\"elementor-element elementor-element-12487e0d elementor-widget elementor-widget-heading\" data-id=\"12487e0d\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">How to Choose Rubber Rollers for Heat and Pressure Contact<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t<div class=\"elementor-element elementor-element-f9a2325 e-con-full e-flex e-con e-child\" data-id=\"f9a2325\" data-element_type=\"container\" data-e-type=\"container\">\n\t\t<div class=\"elementor-element elementor-element-4304fb0b e-con-full e-flex e-con e-child\" data-id=\"4304fb0b\" data-element_type=\"container\" data-e-type=\"container\">\n\t\t\t\t<div class=\"elementor-element elementor-element-6f131d0a elementor-widget elementor-widget-text-editor\" data-id=\"6f131d0a\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p class=\"isSelectedEnd\">A rubber roller used near heat and pressure has to stay stable after the line starts running. Cold hardness, surface feel, or a simple replacement match is not enough for every position.<\/p><p class=\"isSelectedEnd\">On heated nips, laminating sections, drying-after-contact areas, hot film handling points, coating lines, and pressure contact positions, the roller cover is affected by temperature, load, contact time, surface finish, and what it touches. A roller may look normal before installation, then begin to mark the product, collect adhesive, slip, stick, soften, glaze, or compress unevenly after the line warms up.<\/p><p>The first checks are practical: actual roller surface temperature, contact time, nip pressure, product surface sensitivity, release behavior, and the condition of the old roller. For ordinary replacement rollers, these details often give a clear starting direction. For demanding heat and pressure contact, the compound direction, bonding, cover thickness, hardness, surface finish, and roller accuracy need to be matched more carefully.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t<div class=\"elementor-element elementor-element-64fa878 e-con-full e-flex e-con e-child\" data-id=\"64fa878\" data-element_type=\"container\" data-e-type=\"container\">\n\t\t\t\t<div class=\"elementor-element elementor-element-6fee46a elementor-widget elementor-widget-image\" data-id=\"6fee46a\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img fetchpriority=\"high\" decoding=\"async\" width=\"800\" height=\"600\" src=\"https:\/\/wolorin.com\/wp-content\/uploads\/2026\/05\/White-Rubber-Roller-Surface-Inspection.webp\" class=\"attachment-large size-large wp-image-3994\" alt=\"Un trabajador inspecciona la superficie de un rodillo de goma blanca con una linterna de mano.\" srcset=\"https:\/\/wolorin.com\/wp-content\/uploads\/2026\/05\/White-Rubber-Roller-Surface-Inspection.webp 800w, https:\/\/wolorin.com\/wp-content\/uploads\/2026\/05\/White-Rubber-Roller-Surface-Inspection-300x225.webp 300w, https:\/\/wolorin.com\/wp-content\/uploads\/2026\/05\/White-Rubber-Roller-Surface-Inspection-768x576.webp 768w\" sizes=\"(max-width: 800px) 100vw, 800px\"  title=\"How to Choose Rubber Rollers for Heat and Pressure Contact\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t<div class=\"elementor-element elementor-element-563fef79 e-flex e-con-boxed e-con e-parent\" data-id=\"563fef79\" data-element_type=\"container\" data-e-type=\"container\">\n\t\t\t\t\t<div class=\"e-con-inner\">\n\t\t\t\t<div class=\"elementor-element elementor-element-f8bc663 elementor-widget elementor-widget-heading\" data-id=\"f8bc663\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">Temperature and contact time<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-44c9f2e1 elementor-widget elementor-widget-text-editor\" data-id=\"44c9f2e1\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p class=\"isSelectedEnd\">The temperature that matters is the temperature at the roller surface during production. It may be different from the heater setting, oven temperature, metal roll temperature, or the temperature shown on the machine panel.<\/p><p class=\"isSelectedEnd\">Un contacto breve cerca de una fuente de calor y un contacto prolongado bajo carga cerca de una fuente de calor representan condiciones de trabajo diferentes. Un contacto breve suele manifestar problemas a trav\u00e9s de marcas superficiales, cambios en la liberaci\u00f3n o una ligera adherencia. Un contacto prolongado a alta temperatura ejerce mayor presi\u00f3n sobre la compresi\u00f3n, la uni\u00f3n, la recuperaci\u00f3n y la estabilidad superficial.<\/p><p class=\"isSelectedEnd\">A common situation is that the roller runs well at the beginning. After the line warms up, the surface starts to become glossy, tacky, softer than expected, or easier to mark the product. In that case, the cold-state hardness tells only part of the story. The running temperature, contact time, and surface change after running are more useful.<\/p><p class=\"isSelectedEnd\">For dry heat, release, and sensitive product contact, <a href=\"https:\/\/wolorin.com\/es\/material\/solid-silicone-rollers\/\">Rodillos de silicona s\u00f3lida<\/a> are often one direction to check. If the roller also touches adhesive, coating liquid, cleaning solvent, oil, ink, or other media, the direction needs a closer look.<\/p><p>Useful details include actual roller surface temperature after running, product temperature before contact, whether the roller touches before or after drying, contact time, and whether the problem appears immediately or only after the roller warms up.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t<div class=\"elementor-element elementor-element-e6c7a7a e-flex e-con-boxed e-con e-parent\" data-id=\"e6c7a7a\" data-element_type=\"container\" data-e-type=\"container\">\n\t\t\t\t\t<div class=\"e-con-inner\">\n\t\t\t\t<div class=\"elementor-element elementor-element-43c46af elementor-widget elementor-widget-heading\" data-id=\"43c46af\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">Pressure and nip condition<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-70b2ae1 elementor-widget elementor-widget-text-editor\" data-id=\"70b2ae1\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p class=\"isSelectedEnd\">Pressure contact is where many roller problems become visible. A roller in a nip is not just supporting the web. It may be feeding, pressing, bonding, isolating tension, removing air, or creating a controlled contact line between two surfaces.<\/p><p class=\"isSelectedEnd\">Too much pressure can leave pressure marks, stretch film, increase heat build-up, overload the cover, or make small alignment problems show on the product. Too little pressure can cause slipping, weak bonding, bubbles, poor transfer, unstable movement, or uneven winding.<\/p><p class=\"isSelectedEnd\">Para <a href=\"https:\/\/wolorin.com\/es\/function\/pressure-rollers\/\">Rodillos de presi\u00f3n<\/a>, hardness alone cannot decide the direction. A harder cover may reduce deformation, but it can make marks sharper. A softer cover may increase contact area, but it can over-compress under heat and load. The roller has to compress evenly, recover after contact, and keep a stable nip across the working width.<\/p><p class=\"isSelectedEnd\">Check whether the mark appears in the center, at the edge, on one side, or at a repeated distance. A center band, edge mark, one-side mark, and circumference repeat mark point to different checks: pressure balance, crown, parallelism, runout, bearing condition, grinding quality, or local cover damage.<\/p><p>In <a href=\"https:\/\/wolorin.com\/es\/applications\/coating-and-laminating-line-rollers\/\">Rodillos para l\u00edneas de recubrimiento y laminaci\u00f3n<\/a>, heat and pressure often work together. A pressure roller may need to press an adhesive layer, protect the film surface, reduce bubbles, release cleanly, and keep stable contact across the web. If the roller cannot hold these points during running, the finished material will show it.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t<div class=\"elementor-element elementor-element-262f8ec e-flex e-con-boxed e-con e-parent\" data-id=\"262f8ec\" data-element_type=\"container\" data-e-type=\"container\">\n\t\t\t\t\t<div class=\"e-con-inner\">\n\t\t\t\t<div class=\"elementor-element elementor-element-f1adb08 elementor-widget elementor-widget-heading\" data-id=\"f1adb08\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">Surface sensitivity \/ pressure marks<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-0b29828 elementor-widget elementor-widget-text-editor\" data-id=\"0b29828\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p class=\"isSelectedEnd\">Some materials can accept small contact marks. Sensitive web materials cannot. Thin film, coated film, release film, flexible packaging material, battery separator film, foil, coated paper, glossy substrates, and printed webs often show small roller differences very quickly.<\/p><p class=\"isSelectedEnd\">A pressure mark may appear as a dull band, bright line, shallow impression, repeating spot, gloss change, wrinkle starting near the nip, or local sticking after contact. The roller may still rotate normally, but the product surface already shows that the contact is not right.<\/p><p class=\"isSelectedEnd\">The mark pattern is important. A regular repeat mark often points to the roller circumference, local surface damage, runout, or a hard spot. A cross-width band usually points to pressure distribution, crown, parallelism, or nip setting. A mark that becomes worse after heating often points to cover softening, heat build-up, compression change, or surface finish. A one-side mark often points to alignment, uneven load, shaft condition, bearing condition, or pressure balance.<\/p><p class=\"isSelectedEnd\">Para <a href=\"https:\/\/wolorin.com\/es\/applications\/film-converting-rollers\/\">Rodillos para conversi\u00f3n de pel\u00edcula<\/a>, surface condition can be more important than basic movement. The roller may still guide or press the web, but if it leaves marks on the film, the working direction is not suitable for that position.<\/p><p>Old roller photos help a lot here. A glossy pressure band, uneven wear line, sticky edge, hardened area, cracked surface, or repeated local defect on the cover can show where heat, pressure, or media contact is concentrated.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t<div class=\"elementor-element elementor-element-1c96edb e-flex e-con-boxed e-con e-parent\" data-id=\"1c96edb\" data-element_type=\"container\" data-e-type=\"container\">\n\t\t\t\t\t<div class=\"e-con-inner\">\n\t\t\t\t<div class=\"elementor-element elementor-element-aa039ed elementor-widget elementor-widget-heading\" data-id=\"aa039ed\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">Release and sticking behavior<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-cb61ad7 elementor-widget elementor-widget-text-editor\" data-id=\"cb61ad7\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p class=\"isSelectedEnd\">Heat often makes sticking more obvious. Adhesive, coating liquid, ink, plasticizer, hot film, release liner, cleaning liquid, and surface treatment residue can all change how the roller surface behaves during production.<\/p><p class=\"isSelectedEnd\">A release-focused roller should let the product leave cleanly. But the surface still has to match the job. If it is too smooth, the web may slip. If the texture is too open, adhesive, dust, or coating residue may collect. If the cover does not suit the media, the surface may swell, soften, become tacky, crack, or lose its original finish.<\/p><p class=\"isSelectedEnd\">In <a href=\"https:\/\/wolorin.com\/es\/applications\/flexible-packaging-rollers\/\">Rodillos para embalaje flexible<\/a>, release, pressure, heat, and web handling often appear together. A laminating or contact roller may need to avoid sticking while still keeping enough contact to feed, press, or support the web. A surface that looks easy to release is not always the best surface for the line.<\/p><p class=\"isSelectedEnd\">Typical signs include adhesive build-up on one side of the roller, residue in fine surface texture, film dragging near a heated contact point, a glossy or tacky roller surface after running, slipping after cleaning, product lifting away from the roller, or cracks and soft spots on the old cover.<\/p><p>When sticking and heat appear together, check the surface finish, cleaning method, contact media, and pressure condition together. Changing the compound direction alone may not solve the issue if the roller is also overloaded, misaligned, contaminated, or ground to an unsuitable surface.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t<div class=\"elementor-element elementor-element-eb842ca e-flex e-con-boxed e-con e-parent\" data-id=\"eb842ca\" data-element_type=\"container\" data-e-type=\"container\">\n\t\t\t\t\t<div class=\"e-con-inner\">\n\t\t\t\t<div class=\"elementor-element elementor-element-cdb870a elementor-widget elementor-widget-heading\" data-id=\"cdb870a\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">Silicone vs FKM as direction, not fixed answer<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-5511ff0 elementor-widget elementor-widget-text-editor\" data-id=\"5511ff0\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p class=\"isSelectedEnd\">Silicone and FKM are both common directions around heat, but they are used for different working conditions.<\/p><p class=\"isSelectedEnd\">Silicone is usually checked when the main concerns are dry heat, release, low marking, surface protection, and sensitive product contact. It is common around hot film contact, heat sealing, release surfaces, pressure contact, and positions where the product must leave the roller cleanly.<\/p><p class=\"isSelectedEnd\"><a href=\"https:\/\/wolorin.com\/es\/material\/fkm-rubber-rollers\/\">Rodillos de caucho FKM<\/a> are more relevant when heat appears together with oil, solvent, chemical contact, aggressive coating media, or a roller surface that keeps changing after media exposure. In this case, the cover has to handle both temperature and contact media during real production.<\/p><p class=\"isSelectedEnd\">There are also cases where neither silicone nor FKM is the first direction. If the main problem is heavy abrasion, repeated friction, high load, or grip under pressure, a wear-resistant or traction-oriented direction may be more suitable. If the product is very sensitive to pressure marks, surface finish and roller accuracy may matter as much as the compound direction.<\/p><p class=\"isSelectedEnd\">For standard cases, the starting direction can often be confirmed from roller position, temperature, contact media, hardness, and product surface requirement. For higher-demand positions, Wolorin will also check bonding, cover thickness, compression behavior, surface finish, runout, crown, and the old roller failure pattern.<\/p><p>Two rollers can both be silicone or both be FKM, but perform differently on the same line. Compound direction, bonding, curing and processing control, grinding, surface finish, and real load condition all affect the final result.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t<div class=\"elementor-element elementor-element-9550d34 e-flex e-con-boxed e-con e-parent\" data-id=\"9550d34\" data-element_type=\"container\" data-e-type=\"container\">\n\t\t\t\t\t<div class=\"e-con-inner\">\n\t\t\t\t<div class=\"elementor-element elementor-element-2c43e6a elementor-widget elementor-widget-heading\" data-id=\"2c43e6a\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">What operating details to send<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-6a2b28a elementor-widget elementor-widget-text-editor\" data-id=\"6a2b28a\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p class=\"isSelectedEnd\">For heated pressure contact, clear basic information is enough to start. A perfect technical report is not required.<\/p><p class=\"isSelectedEnd\">Si ya dispone de planos, medidas, muestras o especificaciones claras, env\u00edelos directamente. Podemos proceder con la fabricaci\u00f3n a medida, la cotizaci\u00f3n o la confirmaci\u00f3n de producci\u00f3n bas\u00e1ndonos en su documentaci\u00f3n.<\/p><p class=\"isSelectedEnd\">If the information is not complete yet, start with the roller diameter, face length, shaft photos, cover thickness, current hardness if known, roller position, product type, and old roller photos.<\/p><p class=\"isSelectedEnd\">For heat and pressure contact, also send the actual roller surface temperature during running, contact time, nip pressure or load if known, speed range, contact media, and the problem seen on the product. If the issue appears only after the line warms up, mention how long it takes. If the roller works at low speed but fails at higher speed, mention that too.<\/p><p>Photos are useful when they show the whole roller, both shaft ends, close-up surface condition, product marks, adhesive build-up, sticking area, cracks, swelling, hardening, softening, glossy bands, or uneven wear.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t<div class=\"elementor-element elementor-element-ab9ff31 e-flex e-con-boxed e-con e-parent\" data-id=\"ab9ff31\" data-element_type=\"container\" data-e-type=\"container\">\n\t\t\t\t\t<div class=\"e-con-inner\">\n\t\t\t\t<div class=\"elementor-element elementor-element-a7c1d7b elementor-widget elementor-widget-heading\" data-id=\"a7c1d7b\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">Heat and Pressure Contact Review Table<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-d356a4f elementor-widget elementor-widget-text-editor\" data-id=\"d356a4f\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<table><tbody><tr><th>What you see on the line<\/th><th>A lo que suele apuntar<\/th><th>What to check on the roller<\/th><\/tr><\/tbody><\/table><table><tbody><tr><td>Works at startup, marks after heating<\/td><td>Heat softening, compression change, surface change after running<\/td><td>Actual roller surface temperature, hardness after running, cover thickness, surface finish<\/td><\/tr><\/tbody><\/table><table><tbody><tr><td>Dull band or bright line on sensitive film<\/td><td>Pressure concentration, surface roughness, gloss transfer, uneven nip<\/td><td>Pressure balance, crown, runout, grinding, surface cleanliness<\/td><\/tr><\/tbody><\/table><table><tbody><tr><td>Adhesive build-up near heated contact<\/td><td>Poor release, surface texture collecting residue, media mismatch<\/td><td>Surface finish, cleaning method, contact media, silicone \/ FKM direction<\/td><\/tr><\/tbody><\/table><table><tbody><tr><td>One side marks more than the other<\/td><td>Uneven load, alignment issue, shaft or bearing condition<\/td><td>Parallelism, bearing seat, pressure setting, roller end condition<\/td><\/tr><\/tbody><\/table><table><tbody><tr><td>Bubbles or weak bonding after lamination<\/td><td>Low or unstable nip contact, pressure variation, poor surface support<\/td><td>Nip pressure, cover hardness, roller accuracy, web tension near the nip<\/td><\/tr><\/tbody><\/table><table><tbody><tr><td>Product sticks or drags on the roller<\/td><td>Poor release, tacky cover, heat \/ media surface change<\/td><td>Release direction, surface condition, temperature after running, old cover damage<\/td><\/tr><\/tbody><\/table><table><tbody><tr><td>Old roller shows glossy pressure band<\/td><td>Repeated loaded contact, heat and pressure concentration<\/td><td>Contact zone, pressure setting, hardness change, local wear pattern<\/td><\/tr><\/tbody><\/table>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t<div class=\"elementor-element elementor-element-45b150d e-flex e-con-boxed e-con e-parent\" data-id=\"45b150d\" data-element_type=\"container\" data-e-type=\"container\">\n\t\t\t\t\t<div class=\"e-con-inner\">\n\t\t\t\t<div class=\"elementor-element elementor-element-3bfaa32 elementor-widget elementor-widget-heading\" data-id=\"3bfaa32\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">P\u00e1ginas relacionadas<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-b0f8a19 elementor-widget elementor-widget-text-editor\" data-id=\"b0f8a19\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<ul><li><a href=\"https:\/\/wolorin.com\/es\/material\/solid-silicone-rollers\/\">Rodillos de silicona s\u00f3lida<\/a> \u2014 For heat, release, surface protection, and sensitive contact directions.<\/li><li><a href=\"https:\/\/wolorin.com\/es\/material\/fkm-rubber-rollers\/\">Rodillos de caucho FKM<\/a> \u2014 For heat combined with oil, solvent, chemical, or complex media contact.<\/li><li><a href=\"https:\/\/wolorin.com\/es\/function\/pressure-rollers\/\">Rodillos de presi\u00f3n<\/a> \u2014 For controlled nip pressure, compression, pressure marks, and surface contact.<\/li><li><a href=\"https:\/\/wolorin.com\/es\/applications\/coating-and-laminating-line-rollers\/\">Rodillos para l\u00edneas de recubrimiento y laminaci\u00f3n<\/a> \u2014 For heated coating, drying, adhesive, release, and lamination contact points.<\/li><li><a href=\"https:\/\/wolorin.com\/es\/applications\/flexible-packaging-rollers\/\">Rodillos para embalaje flexible<\/a> \u2014 For film, printed web, laminating, pressure contact, release, and surface protection.<\/li><\/ul>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t<div class=\"elementor-element elementor-element-5fefb443 e-flex e-con-boxed e-con e-parent\" data-id=\"5fefb443\" data-element_type=\"container\" data-e-type=\"container\">\n\t\t\t\t\t<div class=\"e-con-inner\">\n\t\t\t\t<div class=\"elementor-element elementor-element-286de4b3 elementor-widget elementor-widget-heading\" data-id=\"286de4b3\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">Fabricaci\u00f3n de rodillos a medida y control de calidad<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-21827b6e elementor-widget elementor-widget-text-editor\" data-id=\"21827b6e\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p data-start=\"186\" data-end=\"393\">Un rodillo de caucho fiable no solo depende de su tama\u00f1o. La direcci\u00f3n del compuesto, la estabilidad de la dureza, el grosor de la cubierta, el acabado superficial, la estructura del eje y la precisi\u00f3n de funcionamiento influyen en el rendimiento del rodillo en la l\u00ednea de producci\u00f3n.<\/p><p data-start=\"395\" data-end=\"675\">Wolorin ofrece servicios tanto para el reemplazo rutinario de rodillos como para proyectos personalizados m\u00e1s exigentes, con procesos de fabricaci\u00f3n, inspecci\u00f3n y controles de calidad documentados que se ajustan a los requisitos de cada proyecto. A continuaci\u00f3n, puede consultar nuestro alcance de servicios, nuestro proceso de control de calidad y nuestra trayectoria empresarial.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t<div class=\"elementor-element elementor-element-1794fb85 e-con-full e-flex e-con e-child\" data-id=\"1794fb85\" data-element_type=\"container\" data-e-type=\"container\">\n\t\t\t\t<div class=\"elementor-element elementor-element-6a496285 elementor-widget elementor-widget-button\" data-id=\"6a496285\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-sm\" href=\"https:\/\/wolorin.com\/es\/services\/\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">Servicios<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-2d19d442 elementor-widget elementor-widget-button\" data-id=\"2d19d442\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-sm\" href=\"https:\/\/wolorin.com\/es\/company\/quality-control\/\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">Control de calidad<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-7bfd0c55 elementor-widget elementor-widget-button\" data-id=\"7bfd0c55\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-sm\" href=\"https:\/\/wolorin.com\/es\/company\/\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">Acerca de Wolorin<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t<div class=\"elementor-element elementor-element-1b344549 e-flex e-con-boxed e-con e-parent\" data-id=\"1b344549\" data-element_type=\"container\" data-e-type=\"container\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t\t\t<div class=\"e-con-inner\">\n\t\t<div class=\"elementor-element elementor-element-6b839eb7 e-con-full e-flex e-con e-child\" data-id=\"6b839eb7\" data-element_type=\"container\" data-e-type=\"container\">\n\t\t\t\t<div class=\"elementor-element elementor-element-3a581bff elementor-widget elementor-widget-heading\" data-id=\"3a581bff\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h2 class=\"elementor-heading-title elementor-size-default\">Solicitar presupuesto<\/h2>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-4fcab6b2 elementor-widget elementor-widget-text-editor\" data-id=\"4fcab6b2\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p class=\"isSelectedEnd\">Si ya dispone de planos, medidas, muestras o especificaciones claras, puede envi\u00e1rnoslos directamente. Podemos proceder con la fabricaci\u00f3n a medida, la cotizaci\u00f3n o la confirmaci\u00f3n de producci\u00f3n bas\u00e1ndonos en su documentaci\u00f3n.<\/p><p>If the information is not complete yet, you can still start with old roller photos, roller position, product type, contact media, actual running temperature, and the current problem seen on the line.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t<div class=\"elementor-element elementor-element-2f30df17 e-con-full e-flex e-con e-child\" data-id=\"2f30df17\" data-element_type=\"container\" data-e-type=\"container\">\n\t\t\t\t<div class=\"elementor-element elementor-element-5bd606c4 elementor-widget elementor-widget-button\" data-id=\"5bd606c4\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-sm\" href=\"https:\/\/wolorin.com\/es\/contact-us\/\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">Contacto<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-87d6223 elementor-widget elementor-widget-button\" data-id=\"87d6223\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-sm\" href=\"https:\/\/wolorin.com\/es\/send-drawings\/\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">Enviar planos o datos del rodillo<\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<\/div>","protected":false},"excerpt":{"rendered":"<p>How to Choose Rubber Rollers for Heat and Pressure Contact A rubber roller used near heat and pressure has to stay stable after the line starts running. Cold hardness, surface feel, or a simple replacement match is not enough for every position. On heated nips, laminating sections, drying-after-contact areas, hot film handling points, coating lines, [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"comment_status":"closed","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"site-sidebar-layout":"no-sidebar","site-content-layout":"page-builder","ast-site-content-layout":"full-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"","ast-breadcrumbs-content":"","ast-featured-img":"disabled","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"set","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"var(--ast-global-color-4)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"categories":[1],"tags":[],"class_list":["post-4239","post","type-post","status-publish","format-standard","hentry","category-blog"],"_links":{"self":[{"href":"https:\/\/wolorin.com\/es\/wp-json\/wp\/v2\/posts\/4239","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/wolorin.com\/es\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/wolorin.com\/es\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/wolorin.com\/es\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/wolorin.com\/es\/wp-json\/wp\/v2\/comments?post=4239"}],"version-history":[{"count":4,"href":"https:\/\/wolorin.com\/es\/wp-json\/wp\/v2\/posts\/4239\/revisions"}],"predecessor-version":[{"id":4243,"href":"https:\/\/wolorin.com\/es\/wp-json\/wp\/v2\/posts\/4239\/revisions\/4243"}],"wp:attachment":[{"href":"https:\/\/wolorin.com\/es\/wp-json\/wp\/v2\/media?parent=4239"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/wolorin.com\/es\/wp-json\/wp\/v2\/categories?post=4239"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/wolorin.com\/es\/wp-json\/wp\/v2\/tags?post=4239"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}